Paint failing on the outside of a building is telling you something specific, and the pattern of the failure usually identifies the cause. Repainting without reading it means repeating it.

Blistering

Bubbles lifting off the surface, sometimes containing moisture.

The cause is almost always moisture behind the film. Either the surface was damp when painted, or water is getting into the wall or timber from somewhere and cannot escape.

On masonry it frequently means an impermeable paint on a wall that needs to breathe.

Occasionally it is heat blistering, where a dark colour in strong sun softened the film.

The fix is to find the water source first: gutters, pointing, copings, ground levels, a bridged damp proof course. Then strip back the affected area, let it dry thoroughly and repaint, using a breathable paint on a solid wall.

Peeling and flaking in sheets

The coating lifts cleanly, frequently taking everything down to bare substrate.

This is an adhesion failure. The surface was dirty, chalky, glossy, damp or unprimed when painted.

Look at the back of a flake. Bare substrate on the underside means it never bonded; another layer of paint means the failure is between coats.

The fix is to remove all loose material, establish why it did not bond, prepare properly and use the right primer.

Where a coating is failing across a whole elevation, it usually all has to come off.

Chalking

A loose powder on the surface that comes off on your hand.

This is normal ageing, as ultraviolet light breaks down the binder and releases the pigment. Cheaper paints chalk sooner.

It is not a defect requiring stripping, and painting straight over it is a mistake, since the new coat bonds to the powder.

The fix is to wash thoroughly, then apply a stabilising solution before repainting.

Cracking and crazing

A network of fine cracks, or deeper cracks following a pattern.

Fine crazing usually means the coating was applied too thickly, or a hard topcoat was applied over a softer or uncured layer.

Cracks that follow the render or the joints below are substrate cracks showing through, not paint failure.

Straight, stepped or widening cracks indicate structural movement, and filling and painting them will not hold. These need investigating.

Mould and algae growing through

Green or black growth appearing within a year or two of painting.

Usually the surface was not treated with a fungicidal wash before painting, so the growth was sealed in and came through.

It also occurs where a wall stays permanently damp and shaded.

The fix is to treat with a fungicidal wash properly, deal with the dampness, and repaint with a paint carrying a strong biocide.

Cutting back overhanging planting helps more than any product.

Colour fade and patchiness

Strong colours, particularly reds, yellows and deep blues, fade faster than neutrals under ultraviolet light.

Patchiness frequently means the surface absorbed unevenly, which points to missed stabilising or an inadequate first coat.

A visible line across a wall usually means a batch change or a stop in the middle of an elevation.

Rust and stains bleeding through

Orange or brown marks appearing weeks after painting.

Rust from a fixing, tannin from timber, or a water stain that was painted over rather than sealed.

The fix is to treat the source, then use a stain blocking primer over the area before recoating.

Working out the underlying cause

Before any repair, ask three questions.

Is water getting in? Check gutters, downpipes, pointing, render cracks, window seals, copings and ground levels.

Could the wall be trapped? An impermeable coating on a solid wall is a common and serious cause.

Was the preparation adequate? Most failures within two years are preparation, not product.

Deciding on the repair

Localised failure can be cut out, feathered, primed and patched, accepting it will show slightly until it weathers.

Failure across a whole elevation means stripping that elevation and starting again.

Repainting over a failing coating buys a season at most, and makes the eventual job larger.