A properly made glue joint in timber is stronger than the timber around it. Getting there depends on the right adhesive, clean surfaces and the right clamping pressure.
PVA wood glue
The standard woodworking adhesive. Water-based, easy to use, cleans up with water before it sets.
Classified by water resistance:
- D2: interior, dry conditions only
- D3: interior, and occasional short-term exposure to water. Suitable for kitchens and bathrooms
- D4: the most water resistant PVA class, suitable for exterior use and frequent wetting
Check the class on the bottle. General purpose white PVA from a decorating aisle is usually D2 and is not the same product as a woodworking D3 or D4.
- Open time typically 5 to 10 minutes
- Clamp for 30 minutes to an hour, full strength in 24 hours
- Cures by water loss, so it needs an absorbent surface and will not cure in a sealed gap
- Does not fill gaps: it shrinks and the joint is weak
- Dries clear to pale, and it will not take a stain, so squeeze-out on a surface to be stained shows as a pale patch
Polyurethane adhesive
A one-part adhesive that cures by reacting with moisture and foams as it does so.
- Very strong, and fully waterproof once cured
- Bonds timber to many other materials: metal, stone, ceramic, some plastics
- Gap filling, since the foam expands into voids, though the foam itself has little strength
- Dampen one surface lightly before applying, since it needs moisture to cure
- It expands considerably, so clamping is essential or it will push the joint apart
- Foam squeeze-out is easiest removed once cured, by paring it off
- Stains skin brown for days and is very difficult to remove. Wear gloves
- Once opened, the bottle has a limited life as moisture gets in
Epoxy
Two parts, resin and hardener, mixed in the stated ratio.
- Very strong, waterproof, and genuinely gap filling with real strength in the gap
- Bonds almost anything to almost anything
- Available in fast set, typically 5 minutes, and slow set with hours of working time
- Slow set epoxies are generally stronger
- Mix thoroughly and in the correct ratio. An incorrect ratio does not cure properly, and no amount of waiting will fix it
- Expensive, so used where its properties are needed
- Excellent for repairs, for oily timbers where PVA struggles, and for bonding dissimilar materials
The others
Cyanoacrylate, superglue. Instant, brittle, and for small repairs and holding parts while another adhesive cures. An accelerator sets it immediately. Bonds skin instantly; keep acetone or a debonder to hand.
Contact adhesive. Applied to both surfaces, left to become touch dry, then brought together.
- Bonds instantly on contact with no repositioning, so alignment must be right first time
- Use dowels or battens as spacers to position a large sheet, removing them progressively
- For laminates and veneers over large areas
- Solvent-based versions need very good ventilation and are flammable
Animal or hide glue. Traditional, reversible with heat and moisture, used in furniture restoration precisely because it can be undone.
Step 1: prepare the joint
Adhesive strength depends on the joint, not just the glue.
- Surfaces must be clean, dry and free of dust, oil and old finish
- Freshly machined or sanded surfaces bond best
- The joint must fit well. PVA does not fill gaps: a joint that needs filling needs epoxy or remaking
- Dry fit everything first, with the clamps, before opening any glue
- Cut and lay out all the softening blocks and clamps in advance
- Note that oily timbers such as teak may need wiping with a solvent first, or an epoxy
Step 2: apply it
- Apply to both surfaces for a strong joint
- Spread evenly with a brush, a roller or a spreader. A thin even film, not a thick bead
- End grain absorbs glue, so size it first with a thin coat, let it soak, then apply properly
- Work within the open time, which is shorter in warm dry conditions
- Mind the temperature: most adhesives have a minimum application temperature, commonly around 5 to 10 degrees
Step 3: clamp correctly
- Assemble and apply clamps hand tight first
- Check square by measuring the diagonals: equal means square
- Check the assembly sits flat and is not twisted
- Tighten evenly, working from the centre outward
- Use softening blocks to protect the work
- Space clamps every 200 to 300mm along a long joint
The right pressure produces a thin even bead of squeeze-out along the whole joint.
- No squeeze-out means too little glue, or too much pressure
- Overtightening starves the joint, squeezing out so much that too little remains
- A starved joint is weak and it looks perfect
Step 4: clean up the squeeze-out
Two approaches, and the wrong one causes trouble.
- Wipe immediately with a damp cloth, rinsing it frequently. Fast, and it can spread thinned glue into the grain where it will resist stain
- Or wait until rubbery, typically 20 to 40 minutes, and pare it off cleanly with a chisel. Neater and the better method on anything to be stained or oiled
- Do not let it set hard, when it must be scraped or sanded off and will have soaked into the grain
- Glue in the grain shows as a pale patch under stain, and there is no cure once it is there
Step 5: curing
- Clamp time is when the clamps can come off; cure time is when the joint reaches full strength. They are different
- Leave clamps on for the stated clamp time, and longer in cold conditions
- Do not stress the joint until the full cure time has passed, typically 24 hours
- Cold and damp conditions slow curing considerably
Step 6: storage and shelf life
- Adhesives have a shelf life and do not work properly beyond it
- Write the date on the bottle when you open it
- PVA is ruined by freezing; store above freezing
- Polyurethane cures in the bottle once moisture gets in; keep the cap tight
- Discard adhesive that has thickened, separated or gone lumpy
If it goes wrong
Joint failed cleanly at the glue line: a starved joint, a contaminated surface, or the glue was past its life.
Joint failed taking timber with it: the glue was stronger than the timber, which is the correct outcome.
Pale patches under stain: glue in the grain. Prevent by paring squeeze-out when rubbery.
Polyurethane pushed the joint open: insufficient clamping against the foaming.
Epoxy still tacky: the ratio was wrong or it was mixed insufficiently. It will not cure. Remove and remake.